| METALLIZED & BARRIER FILMS | METALLIZED PAPER & BOARD | METALLIC YARN | PRODUCTS |
METALLIZED & COATED FILMS |
JALPAC INDIA .... AN EXTENSIVE RANGE OF METALLIZED & COATED FILMS FOR TEXTILE END USES |
| Jalpac's coated
films are used to produce a wide range of metallic yarns. These films provide excellent
machinability during microslitting, resulting in higher productivity and also better yield
per kilogram, because of controlled coating weight. |
|||
|
Silver, Gold and Colours |
I |
Unlacquered Metallized Polyester | 24 micron |
Yarn , Decorative. |
|||
| II | Metallized Polyester Coated on both sides with heat and chemical resistant lacquer | 12 , 24 micron |
Textiles: Weaving and knitting after microstitting into yarn, Twisted Yarn, Zari, Covering. |
|||
| III | Metallized Polyester - High Slip Coated on both sides with heat and chemical resistant lacquer | 24 micron |
Glitter Powder. |
|||
| IV | Metallized Polyester Coated on both Sides. | 24 micron |
Decorative. |
|||
|
||||||
| PROPERTIES | UNITS | TYPICAL VALUES |
||
| Thickness of base film | micron | 12 | 24 | |
| mil | 0.48 | 0.90 | ||
| Grammage | gm/m2 | Silver | 18.6 | 34.5 |
| Gold | 20.4 | 36.5 | ||
| Colour | 20.8 | 36.8 | ||
| Yield | m2/kg | Silver | 54.0 | 28.9 |
| Gold | 49.0 | 27.4 | ||
| Colours | 48.1 | 27.2 | ||
| PROPERTIES | REMARKS |
| Ironing temp (Max.) | 135oC, 15 sec. |
| Dry heat | No change 180oC, 50 sec. |
| Washing | No change Neutral Soap 0.5% |
| 80oC, 15 min. | |
| Steaming | No change 30 min. |
| CHEMICAL RESISTANCE | REMARKS |
| Boiling Water | No change 80oC, 30 min. |
| Ethanol | No change 25oC, 30 min. |
| Trichloroethylene | No change 25oC, 30 min. |
| Benzene | No change 25oC, 30 min. |
| Acetic Acid (5%) | No change 25oC, 30 min. |
| Note: The above specifications are based on tested data by laboratory. | |